Reflow soldering heats the whole assembly through a controlled temperature curve: warm up, soak, melt, cool. Each stage has a job, and each has limits set by the solder alloy and by the most heat-sensitive component on the board. Understanding the profile helps you design boards that solder well and have a useful conversation with your assembler when something goes wrong.

At a glance

217 °C
Approximate melting point of SAC305, the most common lead-free alloy.
235-250 °C
Typical peak temperature range for a lead-free profile.
60-90 s
Typical time above liquidus needed for a sound joint.
260 °C
The peak body temperature many lead-free components are rated to withstand.

The problem

Lead-free solder melts about 34 °C higher than the tin-lead alloy it replaced, which narrows the gap between the temperature needed to form a joint and the temperature that damages parts. A board with both a large connector and tiny passives has to bring them all into that window at once.

Board design changes the result. A pad connected directly to a large copper pour heats slowly and may never reflow properly, while a small part between unequal pads can stand on end, a defect known as tombstoning.

The oven can only compensate so much. Even heating starts with the copper you put on the board.

What designers control

Use thermal relief on pads that connect to planes and pours, so the pad reaches temperature at the same time as its neighbours. Keep the copper on the two pads of small passives balanced.

Tell the assembler about any component with a lower temperature rating than the rest, and about moisture-sensitive parts, which must be stored dry and baked if exposed.

What good looks like

Identify the component with the lowest maximum temperature and the one with the greatest thermal mass. Together they define the process window.

Design pads and thermal reliefs so small and large features heat at similar rates.

Have the assembler profile the actual board with thermocouples rather than relying on a generic recipe.

Stages of a lead-free profile
StageTemperaturePurpose
PreheatAmbient to about 150 °CRaise temperature gradually, up to about 3 °C per second
Soak150-200 °C for 60-120 sEven out temperatures and activate the flux
ReflowAbove 217 °C for 60-90 sMelt the solder and form the joint
Peak235-250 °CEnsure full wetting without overheating parts
CoolingDown at up to about 4 °C per secondSolidify the joint with a fine grain structure
Typical values for SAC305. Follow the solder paste datasheet and component ratings for your build.
Key temperatures
°C
Tin-lead melts183
SAC305 melts217
Typical peak245
Component limit260
Melting points of common alloys and typical process limits, in degrees Celsius.

What it changes

Joint Quality

Correct time above liquidus gives well-wetted joints with a sound intermetallic layer.

Component Safety

Peak temperature stays below the rating of every part on the board.

Yield

Balanced heating reduces tombstoning, cold joints and voids.

Repeatability

A profile measured on the real board carries from prototype to production.

Where to go next

Boards with components on both sides are reflowed twice. Place heavy parts on the side soldered last so they are not held only by surface tension.

If through-hole parts are needed, discuss selective or wave soldering, or pin-in-paste, with the assembler early.

Problems this prevents

  • Cold joints on pads tied to large pours
  • Small passives standing on end
  • Parts exposed beyond their temperature rating
  • A generic profile applied to an unusual board